During specification writing, design teams and EPC contractors routinely face the practical question of which coating weight to assign to a project location. ISO 9223 provides the internationally recognised classification of atmospheric corrosivity into categories C1–C5 (and CX). Matching coating weight to the actual category balances first-cost against service life more reliably than generic "heavy zinc" or "coastal" labels.
Determining the Category
ISO 9223 classifies an atmosphere by the first-year corrosion rate measured on standard metal specimens (carbon steel, zinc, copper and aluminium). When direct exposure data are unavailable, the category can be estimated from the dose-response functions given in the standard. The governing parameters are the temperature–humidity complex (commonly expressed as time of wetness), sulphur dioxide deposition and chloride deposition.
Typical outdoor descriptors drawn from the standard and supporting guidance are:
- C1–C2: dry or cold regions, rural inland sites with very low pollution and short time of wetness.
- C3: urban or light-industrial atmospheres, or coastal zones with low salinity (often several kilometres inland).
- C4: industrial areas with elevated SO₂ (roughly 30–90 µg/m³) or coastal sites with moderate chloride influence (commonly within about 1 km of the shoreline, outside direct splash).
- C5: heavy industrial pollution or high-salinity coastal exposure (closer to breaking waves or with strong onshore winds).
- CX: offshore, direct sea spray or extreme industrial conditions.
Chloride deposition rates fall rapidly with distance from the coast; many coastal transects show the sharpest decline within the first 1–2 km. Local topography, prevailing wind and sheltering by buildings or vegetation further modify the value, so site-specific assessment or conservative assignment is preferred when measured data are absent.
First-year zinc corrosion rates published with the categories are approximately: C2 0.1–0.7 µm/year, C3 0.7–2.1 µm/year, C4 2.1–4.2 µm/year and C5 4.2–8.4 µm/year. These figures are first-year values; long-term rates are lower once corrosion products form, but the category still governs relative severity.


Selecting Pure Zinc (Z) versus Aluminium-Zinc (AZ) Coating Weights
Continuous hot-dip pure zinc coatings are designated by total coating mass on both sides (for example Z120, Z180, Z275). Aluminium-zinc alloy coatings (typically 55 % aluminium, remainder zinc plus silicon) use the AZ designation (AZ100, AZ150, AZ200).
Industry practice, informed by the corrosion-rate bands above and comparative exposure programmes, commonly aligns as follows:
- Z60–Z120 for C1–C2 low-corrosivity interiors or dry rural locations.
- Z180–Z275 for many C3 and moderate C4 sites.
- AZ100–AZ150 for C2–C3 and a substantial portion of C4 applications, where the alloy coating frequently out-performs an equal-mass pure-zinc layer because of the dual barrier-plus-sacrificial mechanism.
- AZ150–AZ200 for more aggressive C4 conditions.
A Z275 coating typically provides roughly 19 µm of zinc per side. An AZ150 coating is of similar or slightly greater thickness because of the lower density of the alloy. In moderate-to-high corrosivity atmospheres the aluminium-rich phase improves barrier performance, which is why AZ grades are frequently preferred once the category reaches C3–C4.
Indicative Environment–Coating–Service-Life Ranges
The ranges below are industry-experience intervals derived from the ISO 9223 first-year rates, published long-term guidance and comparative field observations. They are planning figures only and are not performance guarantees.
| Corrosivity | Typical environment features | Recommended zinc | Recommended Al-Zn | Experience range (bare coating) |
|---|---|---|---|---|
| C2–C3 | Urban / light industrial | Z120–Z180 | AZ100–AZ150 | 15–25 years |
| C4 | Coastal (moderate chloride) or medium industrial | Z275 | AZ150–AZ200 | 10–20 years |
| C5 | High salt spray / heavy pollution | Not recommended alone | AZ200 + colour coating | Dual protection required |
Why Dual Protection Becomes Preferable at C4–C5
At the upper end of C4 and throughout C5 the annual zinc consumption rises sharply. Even a Z275 layer can be substantially depleted within a decade under high chloride or high SO₂ conditions. The sacrificial action of pure zinc remains useful at cut edges and scratches, yet the coating itself is consumed. An organic colour coating applied over the metallic layer supplies a continuous barrier that slows access of moisture and pollutants to the metal. The combination therefore extends the period before first maintenance. For the highest categories the aluminium-zinc substrate (AZ150 or AZ200) plus a suitable paint system is the usual practical specification.


Application in Project Specifications
The approach above is used when writing material specifications for building envelope systems, structural steelwork, warehouses, agricultural buildings and general infrastructure. Once the project location's ISO 9223 category is identified-by reference to distance from the coastline, known industrial pollution levels, local meteorological data or direct measurement-the coating weight (Z or AZ) can be stated together with any requirement for a subsequent organic coating. This produces a clear, auditable line item rather than a generic "galvanized to suit the environment" phrase.
For continuous coil products, detailed product ranges and technical data sheets for pure-zinc galvanized coil and aluminium-zinc (Galvalume-type) coil are available on the relevant category pages. Site-specific coating-weight recommendations can be prepared when the project location and target service interval are supplied.