Why Coating Thickness in Microns Leads to More Disputes Than Coating Mass

Nov 24, 2026

Leave a message

info-800-450

 

Inspection reports reach us with a photograph attached: a magnetic gauge pressed against a galvanized sheet, a reading in the high teens, and a line saying the coating is under specification. In most of the cases we handle, the coil has passed every test the standard asks for. What failed is the figure in the purchase order.

 

Galvanized coating gets described two ways at once. Mills test and certify it by mass, in grams per square metre. Designers, traders and site inspectors usually talk about it in microns. Both refer to the same zinc layer, but only one of them is measured. The other is calculated, and a calculated figure carries assumptions that a contract seldom records.

 

The Coating Mass to Micron Conversion Is Arithmetic

 

Thickness comes from mass divided by the density of zinc. ASTM A653 fixes the factor at 7.14 g/m² per micron on one surface, which matches a zinc density of 7.14 g/cm³.

 

t (µm, one surface) = m (g/m², one surface) ÷ 7.14

 

Nearly every designation in circulation counts both surfaces together. Z275 is 275 g/m² across the two faces, so each face carries about 137.5 g/m², or 19.3 µm of zinc.

 

Table 1. Coating designations and their approximate thickness per surface

Designation

Total mass, both surfaces (g/m²)

Mass per surface (g/m²)

Approx. thickness per surface (µm)

Z100

100

50.0

7.0

Z180

180

90.0

12.6

Z275

275

137.5

19.3

Z350

350

175.0

24.5

Z450

450

225.0

31.5

Z600

600

300.0

42.0

Totals per EN 10346 and ASTM A653M; thickness from the ASTM factor of 7.14 g/m² per micron, assuming an even split and rounding to one decimal place.

EN 10346 works with 7.1 g/cm³ and prints Z275 as approximately 20 µm per face. The ASTM arithmetic gives 19.3 µm. Both numbers are published, both are used in good faith, and they differ by roughly 3.5% before a sample is cut. An order written as "20 µm minimum" therefore sits 0.7 µm above a coil that is exactly Z275. That gap on its own has been enough to hold a shipment.

info-1000-517

Five Reasons the Same Coil Reads Differently

info-722-484

 

 One face or two. Product standards describe both surfaces together; drawings and corrosion calculations usually describe one. A 20 µm requirement per face carries twice the zinc of a 20 µm requirement in total, and the two are easy to mix up when the number is written backwards from a corrosion target. Distribution matters as well. ASTM A653 permits one face of a Z275 coil to fall to 94 g/m², about 13 µm, while the triple-spot average stays at 275.

 Where the reading is taken. The standard defines an average at edge, centre and edge across the width. A gauge placed on one accessible point answers a narrower question. Coating mass varies across the width and down the length of every coil. For Z275 the single-spot floor is 235 g/m², about 16.5 µm per face on an even split, so a compliant coil compared against a 19 µm clause can look short without being short.

 The instrument and its calibration. Magnetic gauges (ISO 2178, ASTM B499) read probe lift-off, and substrate grade, curvature, probe pressure and calibration foils all move the result. X-ray fluorescence (ISO 3497, ASTM B568) measures mass over a small spot against its own references. Microscopy of a prepared cross-section (ISO 1463) reads one plane and has to decide whether the alloy layer counts. Three accepted methods, three different numbers on one coil.

 The density assumed. Zinc-aluminium, zinc-aluminium-magnesium and zinc-iron coatings do not share the density of pure zinc, and within a single hot-dip layer the alloy phase next to the steel differs from the free zinc at the surface. One factor cannot serve all of them, yet the contract rarely says which factor applies.

 Rounding, then tolerance. A 20 µm target becomes 19.3 µm at the first conversion, 19 µm after rounding, and 18.6 µm once gauge tolerance is applied. A threshold set on the calculated value leaves no room for any of it.

 

What a Claim Looks Like From Our Side

 

The pattern repeats. A buyer writes 20 µm minimum into the drawing. We ship DX51D+Z275 and the mill certificate reports 283 g/m², above the designation. His inspector takes five readings with a magnetic gauge calibrated against a different substrate and averages 17.9 µm. The claim cites a 10% shortfall. Our certificate is not wrong, and neither are his readings. They are not the same quantity.

 

It usually ends with a gravimetric retest at a laboratory both parties accept, which returns 279 g/m². The coil is released. What remains is a shipment that waited three weeks, a file of correspondence, and a credit note agreed to preserve the relationship. None of it was about the zinc.

 

Why We Quote in Grams

 

The reference test is a weighing. A specimen of known area is weighed, the coating dissolved in inhibited hydrochloric acid, the steel weighed again, and the difference divided by the area. ISO 1460 and ASTM A90/A90M describe the method; ASTM A924 fixes where the samples come from.

 

There is no proprietary step in that chain. A 100 × 100 mm coupon at 275 g/m² carries about 2.75 g of zinc, which a 0.01 g balance resolves comfortably. Two laboratories working from the same coupon should land within a few grams of each other, and the figure they produce is the one already on the certificate and in the standard.

 

Commercially, that changes the conversation. A micron clause invites a measurement contest at destination, where the buyer holds the instrument and the seller holds the certificate. A mass clause moves the question to a sample, a balance and a method both sides have already agreed.

 

How We Recommend Writing the Requirement

 

Our sales and technical teams review coating clauses before quotation. This is the form we suggest:

 

"Hot-dip galvanized steel coil to EN 10346, grade DX51D+Z275, coating mass 275 g/m² minimum triple-spot average, total on both surfaces, tested in accordance with ISO 1460; approximately 20 µm per surface, for reference only."

 

The same points apply to an enquiry, a technical agreement or a framework contract:

 

 Name the product standard and its edition, not only the coating designation.

 State the designation and say that the number is a total for both surfaces.

 If one face needs more protection, give it a separate mass requirement rather than a micron figure.

 Name the test method and sampling positions, and say what the certificate should show.

 Keep the micron value as a note for the drawing office and mark it approximate.

 Agree the referee laboratory and the retest procedure before the coil ships.

 

Table 2. How the three common ways of writing a coating requirement compare

Specification approach

Verifiability

Dispute risk

Recommended use

Coating mass (g/m²)

High: gravimetric, reproducible by both parties

Low

Primary specification in PO and contract

Coating thickness (µm)

Medium: method, calibration and location dependent

High

Internal reference or approximate description

"Thick zinc layer" only

Low: no defined quantity or test method

Very high

Not recommended

Where Microns Still Earn Their Place

 

Thickness remains useful in engineering. Coating has to be added to substrate thickness in a stack-up. Clearance, welding settings and paint pre-treatment depend on it. Service life is estimated from zinc loss rates against ISO 9223 corrosivity categories, and that estimate starts in microns. On the line, today's gauge reading compared with last month's is a useful trend. None of those uses requires the micron figure to become an acceptance criterion.

 

Before You Send the Enquiry

 

If a drawing already carries a micron figure, we will convert it, tell you what coating mass it implies and quote against that mass instead. If you are revising a contract, we will mark the clauses that cannot be tested as written.

 

Our hot-dip galvanized coil range is supplied against Z100 to Z600 and the ASTM equivalents, with coating mass, mechanical properties and surface treatment reported on the certificate. The coating mass and thickness reference carries the full conversion table, and our technical team will review a specification before it reaches the quotation stage.

 