A coated coil certificate often arrives as one line of text: "Salt spray 500 h, no red rust." For many buyers that line is the whole of the evidence, and it says almost nothing about what 500 hours of salt spray means for the coil in front of them.

 

We produce and export hot-dip zinc-coated, 55% aluminium-zinc-coated and colour-coated steel coil, mostly for buyers in Africa, South-East Asia and Central Asia. A good part of our technical correspondence is spent reading certificates that other mills issued. The figure usually carries some information. It rarely carries what the buyer assumes, and the gap is seldom deliberate. Reports arrive abbreviated because the test house abbreviated them.

 

What was run, and on which method

 

Salt spray is a family of tests, not one test. Two references dominate. ASTM B117, Standard Practice for Operating Salt Spray (Fog) Apparatus, and ISO 9227, Corrosion tests in artificial atmospheres, Salt spray tests. ISO 9227 covers neutral salt spray (NSS), acetic acid salt spray (AASS) and copper-accelerated acetic acid salt spray (CASS). Each attacks a zinc surface at a different rate, so hours from one variant cannot be read against hours from another.

 

Neutral salt spray is the working reference for coil. Under ISO 9227 the usual conditions are 50 g/L sodium chloride, a collected solution pH of 6.5 to 7.2, a chamber temperature of 35 °C, and fog applied without interruption. A report that leaves out these values gives the reader no way to check that the run matched the standard.

 

Duration needs a second look as well. A 500-hour exposure that leaves a Z275 surface unchanged has shown that the chamber ran correctly and that the coating held. It has not shown where that coating's limit sits. Ask what duration would have produced first red rust, and whether anyone ran that far. The answer often settles the question faster than the certificate did.

 

What counted as failure

info-360-360
info-379-379

Most salt spray methods describe how to run the test and stop there. ASTM B117 states that it prescribes neither specimen preparation, test duration, nor the interpretation of results. The pass or fail line therefore comes from elsewhere: a product standard, a purchase specification, or a rating scale agreed before the panels went into the cabinet.

 

In coated steel the line is usually drawn between white rust and red rust. White rust is the corrosion product of the zinc or aluminium-zinc layer and appears first. Red rust means the coating has been breached and the steel beneath is corroding. Buyers normally specify red rust, either absent on the flat surface or limited to a measured width beside a scribe. Prepainted coil is judged on scribed panels, typically to ASTM D1654, with rusting and adhesion read to ASTM D610 and ASTM D3359.

 

A usable criterion is quantitative and dated. No red rust on the unscribed area, red rust within 2 mm of the scribe, white rust below 5% of the surface, assessed at 500 hours to ASTM D1654: that is a sentence a buyer can check. "Passed" alone is not, and neither is a rating level with no scale named beside it.

 

What was actually on the panel

 

Specimen preparation decides what the hours measure. A panel sheared from a coil carries bare steel at the cut edge. Leave that edge unprotected and rust appears there long before the flat surface gives way, so the test ends up grading edge geometry instead of coating quality. A scribe through to the substrate is a different matter, since it is an intentional defect and its width belongs in the report.

 

We expect a report to name the substrate and the coating designation, for instance Z275 to ASTM A653/A653M or ISO 3575, or AZ150 to ASTM A792/A792M, with the measured coating mass and the position where it was taken. It should say how the specimen was cut, whether edges were masked, whether a scribe was applied and by what method, how many replicates ran, and whether a reference panel of known performance went into the same cabinet.

 

Replicate count is not a formality. One panel can meet a criterion by luck, and a report with no stated number of specimens cannot carry a claim about a batch.

 

What is there to compare it against

 

One accelerated figure is one point in one environment. Cyclic tests alternate wet, dry and salt stages. ASTM G85 includes modified salt spray procedures such as Prohesion, ISO 11997-1 covers cyclic wet and dry exposure, and SAE J2334 is used for cosmetic corrosion on automotive material.

 

Outdoor panels supply the other half of the picture. Exposure to ISO 8565 or ASTM G50 at sites classified to ISO 9223 lets accelerated hours be set against observed metal loss. A supplier who can show the same substrate in a neutral salt spray run and a cyclic run, or who holds field panels from a classified site, is handing the buyer something to reason with.

 

The opposite case is a single NSS figure carried across a whole catalogue, with no reference material and no stated purpose. That is a marketing number rather than a test result.

 

Table 1. What a documented answer contains, and what should prompt further questions

What to ask

A documented answer

An answer that needs chasing

Test method

Names ASTM B117 or ISO 9227 and the variant, with operating values and the chamber record

Refers only to salt spray testing, with no standard number and no operating data

Failure criterion

Sets red rust or white rust limits, the rating procedure and the assessed area

States that the material passed, or gives a level without naming the scale

Specimen

Records coating designation, measured mass, edge treatment and scribe method

Leaves edge preparation, scribe and replicate count unstated

Supporting data

Adds cyclic testing or classified outdoor exposure on the same substrate

Offers one neutral salt spray figure for the entire range

 

Why the hours do not become years

 

A chamber holds one set of aggressive conditions steady. Service does the reverse. It wets and dries, carries chloride and sulphur compounds, sees ultraviolet light, and swings in temperature. Coating loss responds to all of that, which is why no published factor converts salt spray hours into years of outdoor life. A supplier who quotes such a factor should be asked where it comes from.

 

What can be estimated is the coating. ISO 9223 gives first-year zinc corrosion rates by category, from below 0.1 µm per year in C1 to above 10 µm per year in CX. Pair a measured coating mass with a site category and the result is a service estimate with visible assumptions, which is more use than a chamber figure dressed up as one. A salt spray result is evidence that the line is consistent. It is not a stand-in for the estimate.

 

How these questions get used

 

They come up in supplier qualification, in tender comparison, and most often when a certificate looks impressive and vague at the same moment. Putting the four questions in an email costs a few minutes. The reply is usually the first technical document of any substance that a buyer gets from a mill, and evaluating a salt spray certificate becomes a matter of checking stated criteria rather than weighing up adjectives.

 

Our product pages carry a testing and inspection module setting out the standards, coating designations and reporting format we apply to each family of coil. Certificates issued by other suppliers can be sent to us for written comment on what they do and do not establish. Sample reports and our full inspection protocol are available on request.

 