Three photographs arrive with the claim: a close-up of brown corrosion at the bore, no mill tag in the frame, no date. Nothing in them can be measured against a specification, and the claim stalls at the first exchange. Planning the documentation before the container is opened costs less than reconstructing it afterwards. What follows is the coil eye rust claim evidence standard we apply, and the order in which to gather it.
What red rust at the eye actually tells you
The coil eye is the bore at the centre of the coil. On a hot-dip galvanized coil the zinc coating covers the faces; the cut edge carries only what the coating line can deposit there, a small fraction of the face coating weight, and the bore exposes that edge along the full length of the strip. Moisture sitting inside the eye has unprotected steel to work on, and red oxide follows.


Red rust and white rust are not the same finding. White rust is zinc corrosion product on the coated face, and it points to moisture trapped between wraps under poor ventilation. Red rust means the substrate is corroding: either the coating was breached where you see it, or the edge stayed wet long enough for the steel underneath to go.
Three measurements decide most of these claims. How far the corrosion runs along the bore. How deep it penetrates in from the edge. Whether it has crossed onto the coated face. Photographs that cannot answer those three turn the discussion into an argument about impressions.
Some edge staining is accepted in the trade. EN 10346 and ASTM A653 set coating and mechanical requirements; neither defines a photographic rust threshold. Surface condition limits are negotiated into the sales contract or the agreed inspection standard. Read that clause before you photograph anything, because the tolerance decides whether there is a claim at all.
Put the coil in the frame, not just the rust
Start wide. Full coil face, both edges, mill tag or coil number legible in the same frame. The tag ties the image to a coil, a heat number and a specific wrap. Without it the photographs belong to no particular coil in the consignment, and the file has no anchor.
The bore supplies a scale reference for free. A 508 mm bore shot from about 300 mm lets a reviewer judge size without a rule in frame. If you add a tape, keep it in the plane of the surface; a tape laid across the bore at an angle reads short.
Shoot both ends where both are accessible. Eye corrosion is rarely symmetric. Condensate collects on the lower bore surface, and the upper surface can stay clean for weeks. Two faces also close off the usual carrier argument that the moisture pattern proves something about stowage.
Then photograph the packaging as found: bore protector, desiccant sachet, VCI paper, edge protectors, all in place. Whether a desiccant was fitted decides causation in many eye rust disputes, and once the sachet is in the skip nobody can answer the question.
How to photograph coil rust for a claim: three angles, one torch
Plan three views, because no single one shows extent and depth together.
The first is square to the face at 1.5 to 2 m, whole face in frame, no digital zoom, edge line kept straight. It shows how much of the bore is affected and where along the circumference the corrosion sits.
The second is at 30 to 45 degrees with a steel rule alongside, close enough to resolve the texture of the oxide. Take it twice: once with a torch held almost parallel to the surface, once under diffuse light. Raking light shows whether there are pits beneath the rust. Frontal flash does not, and a one millimetre pit photographs the same as a one millimetre film of oxide.
The third puts affected and sound metal in one frame, at the same distance and under the same lighting, on the same coil. That is the frame a third party uses to judge how far the corrosion extends and whether the edge zone is the only area involved.
Video, if you record it, should run in one take from the door seal through devanning to the opened eye, with date and time visible. Cut footage invites the question of what happened between takes.
Fix the time
Rust photographed on the first working day and rust photographed on the thirtieth point to different origins, and the difference decides who pays. Open the container in daylight if possible and shoot the same day. Record the hour as well as the date; condensation follows the temperature swing, not the calendar.
Use two time references. File metadata is the first, and it survives only if you export originals; resizing, compressing or forwarding through a messaging application strips EXIF data without warning. The second is something visible in the frame, such as the container number and seal number, or a written date card held beside the coil. A visible marker survives any compression and reads the same in any jurisdiction.
State the time zone once in the report. 09:14 in Rotterdam and 09:14 in Shanghai are eleven hours apart.
Do not clean the surface before documenting it. The corrosion product is the sample. If a laboratory test is needed, photograph, sample, photograph again, and record the chain of custody.
Evidential weight by item
|
Evidence item |
What the reviewer looks for |
Weight |
What usually goes missing |
|
Coil identification |
Mill tag or coil number legible in the same frame as the defect |
High |
Close-ups with no tag |
|
Extent and depth |
Affected arc length on the bore, penetration in millimetres, spread onto the coated face |
High |
Extent described in words only |
|
Angles and lighting |
Square view, angled close-up, raking light, comparison with sound metal |
High |
One angle, flash only |
|
Time reference |
Same working day as devanning, metadata plus visible marker |
High |
No date, metadata stripped |
|
Process record |
Continuous video or sequence of unstuffing and opening |
Medium to high |
Static photographs only |
|
Packaging retention |
Protectors, desiccant and VCI photographed in place and kept |
Medium to high |
Packaging discarded before survey |
|
Transit records |
Container condition, seal number, dunnage, carrier correspondence |
Medium |
Container not inspected at discharge |
Three correct frames outweigh thirty frames of rust. The table is a checklist, not a ranking of effort.
Where the file usually breaks
Galvanized coil damage documentation fails on the same four points: no tag in frame, one angle, no time reference, packaging already gone. None of these is a corrosion finding. All are documentation failures, and none can be repaired after the coil is opened.
Two procedural points matter as much as the photographs. The notice period in your contract normally runs from discharge, not from the day the container is finally opened, so open it early even if the buyer is not ready to inspect. A joint survey arranged before unpacking outweighs unilateral images from either side, because both parties sign the same record.
Keep the transit side of the file as well: container internal condition, floor moisture, dunnage, door seal integrity, and any letter of protest to the carrier. If the container was wet, that is a separate line of recovery with its own evidence.
The mill documents that pair with your photographs are the certificate to EN 10204 3.1, the packing list, the pre-shipment eye photographs taken before the bore protector was fitted, and the desiccant specification for the voyage. Request them by coil number. Matching both ends of the shipment is what turns a set of images into a case.
A sequence to follow on arrival
Photograph the door seal and container number before opening anything.
Record the date, the time and who is present.
Photograph the container interior, dunnage and any moisture on the floor.
Locate the coil tag, then shoot the full face.
Photograph the packaging in place, remove it, then photograph the bore.
Work through the three angles, raking light included, with a scale in frame.
Bag the packaging and desiccant, label them with the coil number, store them dry.
Send notice to your supplier and the carrier within the contract window.
The sequence takes about half an hour per coil and settles most of the questions a surveyor would otherwise raise later. For a one-page version to keep in the warehouse, download our claim evidence checklist. It is written to sit alongside the packaging specification for galvanized coil and the quality documentation covering coating weight, edge condition and bore protection. Read the packing requirements before the container is loaded, and the evidence requirements before it is opened; both describe the same standard from opposite ends of the voyage.